Skip to main content

Table 3 Physical and mechanical properties of dried E. globoidea veneers

From: Properties of rotary peeled veneer and laminated veneer lumber (LVL) from New Zealand grown Eucalyptus globoidea

 

Dried density (kg/m3)

Moisture content (%)

Shrinkage (%)

Velocity (km/s)

Dynamic MoE (GPa)

Mean

688.13

7.31

9.85

4.657

15.14

SD

68.55

1.09

0.77

0.240

2.05

Min

557.41

5.51

8.46

4.322

11.04

Max

824.00

9.32

11.31

5.097

19.51